際際滷

際際滷Share a Scribd company logo
DevelopmentofMasonryCement&Ready足MixMortarforSaurashtra
CementLimitedRanavav,Gujrat
STRENGTHWITHHATHICEMENTMIX


Grad
e

Cemen
t
F/
A
Lime
Ston
e
Consiste
ncy I.S.T. F.S.T
3Days
Strength(MPa)
7Days
Strength(MPa)
28Days
Strength(MPa)
M1 214 53 133 32.00%
105
Min.
210Min. 11.64 15.61 22.45
M2 183 46 171 33.50% 100Min 198Min. 7.24 9.75 16.74
M3 160 40 200 34.00% 75Min. 205Min 7.04 7.877 15.577
M4 142 36 222 34.50% 89Min. 226Min. 5.777 7.188 13.31
Hathi 400 0 0 27.00% 94Min. 173Min. 35.88 38.16 54.97

STRENGTHWITHACCCEMENTMIX

Grade
Cemen
t
F/
A
Lime
Ston
e
Consiste
ncy I.S.T. F.S.T
3Days
Strength(MPa)
7Days
Strength(MPa
)
28Days
Strength(MPa)
A1 214 53 133 32.00% 87Min. 197Min 17.31 20.68 26.98
A2 183 46 171 33.50% 82Min. 218Min 12.29 14.57 19.76
A3 160 40 200 34.50%
83Min. 206
Min.
9.28 11.6 15.67
A4 142 36 222 35.00% 73Min
201
Min.
7.49 9.81 13.54

SIEVEANALYSISOFSAND
I.S.Sieve
(mm)
Average
Cumulative
weight retained
(g)

Cumulative
weight
retained (%)

%Passing
4.75 0 0 100
2.36 7 1.4 98.6
1.18 129 25.87 74.13
0.6 294 58.96 41.04
0.3 438 87.83 12.17
0.15 484 97.06 2.94
Pan 498.67 100 0

STRENGTHAFTERDUSTREMOVALFROMSAND

Mark Cement F/A
Lime
Stone
Admixture
Sand
Qty.Of
Water
7DaysStrength(MPa
CM1       22.94
FM1       18.101



STRENGTHREPORTINDIFFERENTRATIO
Mar
k
Cement F/A
Lime
Stone
Admixture(g
)
Sand
Qty.Of
Water
3Days
Strength(MPa)
7Days
Strength(MPa)
28Days
Strength(MPa
PP足1 800 200 750 2 6000 1335 2.89 4.29 
PP足2 800 200 750 2 6000 1185 3.28 4.78 
PP足3 850 150 750 2 6000 1185 3.23 4.18 
PP足4 800 200 750 2 6000 1185 3.13

More Related Content